Material Light yield (photons/keV) Light ouput of NaI(Tl) (%) Decay time (ns) Wavelength of max emission lm(nm) Refractive index at lm Thickness to stop...
Inorganic Scintillators Physical Properties
Material Light yield (photons/keV) Light ouput of NaI(Tl) (%) Decay time (ns) Wavelength of max emission lm(nm) Refractive index at lm Thickness to stop 50% of 662 keV photons (cm) Hardness (Mho) Density (g/cm3) Hygroscopic BaF2 Barium Fluoride 1.8 fast 3 fast 0.6-0.8 fast 220 fast 1.54 1.9 3 4.88 slightly 10 slow 16 slow 630 slow 310 slow 1.5 BGO Bismuth Germanate 8~10 15~20 300 480 2.15 1 5 7.13 no CaF2(Eu) Europiu...
- ManufacturerOST Photonics
- CategoryScintillator
- Lead TimeQuoted per order
- CustomizationSize, orientation and surface finish to drawing
Physical Properties of Inorganic Scintillators
| Material | Light yield (photons/keV) | Light ouput of NaI(Tl) (%) | Decay time (ns) | Wavelength of max emission lm(nm) | Refractive index at lm | Thickness to stop 50% of 662 keV photons (cm) | Hardness (Mho) | Density (g/cm3) | Hygroscopic |
| BaF2Barium Fluoride | 1.8 fast | 3 fast | 0.6-0.8 fast | 220 fast | 1.54 | 1.9 | 3 | 4.88 | slightly |
| 10 slow | 16 slow | 630 slow | 310 slow | 1.5 | |||||
| BGOBismuth Germanate | 8~10 | 15~20 | 300 | 480 | 2.15 | 1 | 5 | 7.13 | no |
| CaF2(Eu)Europium-doped Calcium Fluoride | 19 | 50 | 940 | 435 | 1.47 | 2.9 | 4 | 3.18 | no |
| CdWO4Cadmium Tungstate | 12~15 | 30~50 | 14000 | 475 | 2.2-2.3 | 1 | 4-4.5 | 7.9 | no |
| CeBr3Cerium bromide | 60 | 157 | 20 | 360~380 | — | — | — | 5.1 | yes |
| CsI(Na)Sodium activated Cesium Iodide | 41 | 85 | 630 | 420 | 1.84 | 2 | 2 | 4.51 | yes |
| CsI(Tl)Thallium activated Cesium Iodide | 54 standard | 45 standard | 1000 | 550 | 1.8 | 2 | 2 | 4.51 | slightly |
| 48 low afterglow | 40 low afterglow | ||||||||
| GAGG(Ce)Cerium-doped Gadolinium Aluminium Gallium Garnet | 54 high light output | — | <150 | 520 | 1.9 | — | 8 | 6.6 | no |
| 45 low afterglow | <70 | ||||||||
| 30 fast decay time | <50 | ||||||||
| 42 balanced | <90 | ||||||||
| GOS CeramicsGadolinium Oxysulfide Ceramic | 27 | — | 3000 | 510 | — | — | — | 7.34 | no |
| LaBr3(Ce)Cerium- doped Lanthanum Bromide | 63 | 165 | 20 | 380 | 1.9 | 1.8 | 2 | 5.1 | yes |
| Li-6 GlassLithium-6 Glass | — | 12 | 53 | 416 | — | — | — | 2.3 | no |
| LSO(Ce)Cerium-doped Lutecium Silicate | 27~30 | 75 | 40 | 420 | 1.82 | 1.15 | 5.8 | 7.4 | no |
| LuAG(Ce)Cerium-doped Lutetium Aluminum Garnet | 25~30 | 20 | 50~70 | 510~550 | 1.84 | 1.3 | 8.5 | 6.73 | no |
| LuAG(Pr)Praseodymi-doped Lutetium Aluminum Garnet | 16~20 | — | 20 | 310 | — | — | 8.5 | 6.73 | no |
| LYSO(Ce)Cerium-doped Lutetium Yttrium Silicate | ~32 | — | 40~44 | 420 | 1.82 | 1.1 | 5.8 | 7.4 | no |
| NaI(Tl)Thallium activated Sodium Iodide | 38 | 100 | 250 | 415 | 1.85 | 2.59 | 2 | 3.67 | yes |
| Pure CsIPure Cesium Iodide | 2 | 4~6 | 16 | 315 | 1.95 | 2 | 2 | 4.51 | slightly |
| YAG(Ce)Cerium- doped Yttrium Aluminum Garnet | ~18 | 40 | 70 | 550 | 1.82 | 2 | 8.5 | 4.55 | no |
| YAP(Ce)Cerium- doped Yttrium Aluminum Perovskite | ~25 | — | 28 | 370 | 1.95 | 2.7 | 8.5 | 5.4 | no |
| YSO(Ce)Cerium- doped Yttrium Silicate | ~28 | — | 50~70 | 420 | 1.8 | — | — | 4.5 | no |
Request A Quote For Inorganic Scintillators Physical Properties
Send us your dimensions, orientation, surface finish and quantity. Our engineers reply with a technical proposal and price.
Buyer Questions
How do I get a quotation for the Inorganic Scintillators Physical Properties?
Can the Inorganic Scintillators Physical Properties be made to a custom specification?
Who manufactures the Inorganic Scintillators Physical Properties?
Tell Us What You Need
Send your specification, quantity and destination port. Our engineers reply with a technical proposal and a confirmed lead time.